1. … °C and the deposition rate is 20-30% higher than with comparable tube metal. It is easy to use and inexperienced welders will have no … matters. Use a larger tip than is generally recommended for same diameter mild steel. Use slight excess acetylene feather. The deposit is …
  2. … Fully austenitic weld metal with high resistance against stress corrosion cracking and … Ni, Mo and Cu. Sufficient resistance against oxidizing acids. The weld metal is corrosion resistant in sea water. CEWELD® SA Alloy 825 is best …
  3. … Catering faciliteiten Het Welding Solution Center werkt nauw samen met gerenommeerde culinaire cateraars die zorg en aandacht besteden aan … voor u en uw klanten zorgt. Accommodatie Binnen een straal van 15 kilometer bevinden zich diverse hotels. Ideaal voor bezoekers uit het … en logistiek Het Welding Solution Center is gemakkelijk bereikbaar met de belangrijkste transportmiddelen en heeft toegang voor het …
  4. … Due to the high resistance to cracking and toughness, all weld metal requires no buffer layer. Suited for wear parts subject to heavy … and shock. The interpass temperature should be maximum 250ºC. The weld metal is machinable with carbide tip tools, hardening is possible. The maximum hardness is dependent on the base metal and is usually already achieved in the first layer. … Rebuilding …
  5. … a slightly higher percentage of phosphor, suitable for MIG welding, easy to handle, high plasticity of the weld metal. High quality alloyed copper wire. The weld metal is a Copper-Silver alloy. Sound, pore free deposits and high …
  6. … a slightly higher percentage of phosphor, suitable for MIG welding, easy to handle, high plasticity of the weld metal. • High quality alloyed copper wire • The weld metal is a Copper-Silver alloy • Sound, pore free deposits and high …
  7. … Due to the high resistance to cracking and toughness, all weld metal requires no buffer layer except on materials considered critical. … and shock. The interpass temperature should be maximum 250ºC. The weld metal is machinable by special carbide tools, hardening is possible. The maximum hardness is dependent on the base metal and is achieved in the first layer. For material considered …
  8. … Due to the high resistance to cracking and toughness, all weld metal requires no buffer layer except on materials considered critical. … and shock. The interpass temperature should be maximum 250ºC. The weld metal is machinable by special carbide tools, hardening is possible. The maximum hardness is dependent on the base metal and is achieved in the first layer. … 55-62 HRc, T Fe2   … AA …
  9. … CEWELD® NiCu30Mn is a Nickel - Copper weld metal and has properties similar to “Monel 400”. It has good strength … in many media, including sea water, salts and reducing acids. The weld metal is not age hardenable and when used to join Monel K-500 it has lower strength then the base metal. … 2.4360, 2.4375, NiCu30Fe, NiCu30Al, Monel alloy 400, R405, …
  10. … offers very good resistance against abrasion by minerals, all weld metal requires no buffer layer except on materials considered critical … temperature should be kept at 270ºC for the best results. The weld metal is only machinable by grinding. Due to the production method (seamless wire) this wire can be stored for a long time without …