1. … cleaned prior to welding. Heavy parts and thicker plates should be preheated (150°C), prior to welding The alloy shows good …
  2. … temperatures up to 600°C. The weld metal is resistant to high hydrogen pressure. … 12crmo19.5, GS-12crmo19.5, 1.7362, 1.7363     … E CrMo5 … A …
  3. … The weld puddle is amazingly fast freezing and therefore especially preferred in vertical down position with high speed and deep …
  4. … cleaned prior to welding. Heavy parts and thicker plates should be preheated (150°C), prior to welding  … Cast aluminium special repairs, …
  5. … current, non conductive coating and a powerful arc at very low amps. Preheating is normally done to slow down the cooling speed, in case you …
  6. … risk of braking out or chipping of. In case of sensitive base material preheating is recommended at 300-400°C. … 600 HB, T Fe 8 … MA 600 …
  7. … alloys and covers a huge range of alloys. Thicker sections should be preheated (150°C) prior to welding. … Aluminium alloys: AlMg4,5Mn, …
  8. … μm FSSS Apparent density (ISO 3923-2) 5.2-5.8 g/cm³ Particle shape: preponderantly spherical Coating microhardness: 800-1300 HV0.3 Sales … 3.3): -45+22 μm (*other sizes on request) -38+15 μm -25+10 μm … Compressor shafts, pump seals, flap actuators, paper rolls, ball valves, …
  9. … to enhance properties. Low carbon (C) helps minimize grain boundary precipitation to maintain corrosion-resistance in the heat-affected …
  10. … and well suited for low-temperatures, ductility down to -60°C. Preheating, interpass temperature and post weld treatment as required …